Scale formation on the Ni-base superalloys IN 939 and IN 738 LC
Scale formation on the Ni-base superalloys IN 939 and IN 738 LC
复制标题
镍基高温合金 IN 939 和 IN 738 LC 上氧化皮的形成
DOI:
10.1007/bf00664797
复制
发表时间:
1989
影响因子:
2.2
通讯作者:
J. Weiss
中科院分区:
文献类型:
--
作者:
J. Litz;A. Rahmel;M. Schorr;J. Weiss
The scales formed on the superalloys IN 939 and IN 738 LC at 700, 900, and 1100°C in air have been investigated by optical, microprobe analysis and x-ray diffraction measurements. Both alloys form very similar scales. The main components are an outer TiO2 layer, an intermediate Cr2O3 layer with dissolved Ti, and an inner layer of (Ti, Nb, Ta)O2 with rutile structure. Beneath the scale an internal corrosion zone is formed that contained Al2O3 directly beneath the external scale and TiN further into the substrate.