Preparation of Fe-Pt-Si Amorphous Ribbons and Their Coercivity after Crystallization
Preparation of Fe-Pt-Si Amorphous Ribbons and Their Coercivity after Crystallization
复制标题
DOI:
10.2320/matertrans.48.74
复制
发表时间:
2007
影响因子:
1.2
通讯作者:
Tokujirou Yamamoto;A. Omori;A. Makino;A. Inoue
中科院分区:
文献类型:
--
作者:
Tokujirou Yamamoto;A. Omori;A. Makino;A. Inoue
Fe x Pt y Si z (x = 60-90, y = 10-70, z = 10-40) ribbons were prepared using a melt-spinning technique. Fully amorphous ribbons were obtained for alloys containing approximately 20-30at%Si. Crystallization of the amorphous ribbons yielded composite structures of L1 0 FePt and Pt-Si intermetallic compounds for Fe 45 Pt 35 Si 20 and Fe 47 Pt 28 Si 25 . Fe 45 Pt 35 Si 20 amorphous ribbons were annealed at 700K for 180min, producing a grain size of approximately 40 nm in diameter, and a maximum coercivity of 160kA/m.