The Study on Leaching Vanadium from Stone Coal with Alkali

The Study on Leaching Vanadium from Stone Coal with Alkali
复制标题

DOI:
--
复制
发表时间:
2007
期刊:
Nonferrous Metals
影响因子:
--
通讯作者:
Shao Yan-hai
Shao Yan-hai
中科院分区:
其他
文献类型:
--
作者:
Shao Yan-hai

文献摘要

被引文献

相似文献

采用球团-氧化焙烧-碱浸工艺从石煤中提钒,考察了焙烧温度、焙烧时间、浸出温度、浸出剂浓度、浸出时间对浸出率的影响。结果表明,焙烧温度、浸出温度、浸出剂浓度、浸出时间是影响石煤中钒浸出率的主要因素。最佳工艺条件为:焙烧温度85 0℃,焙烧时间3 h,浸出温度90℃,浸出剂浓度2 m ol/L,浸出时间2 h,浸出时间2 h。浸出L/S为3。
This study used the technique of pelletization-oxidation roasting-alkali leaching to extract vanadium from stone coal,the effects of roasting temperature,roasting time,leaching temperature,leaching agent concentration,leaching time,leaching L/S were investigated.With this technique,it has got a result of leaching rate was as high as 88.38%.The results indicate that roasting temperature,leaching temperature,leaching agent concentration,leaching time were the main factors which affect the leaching rate.The best technique condition is: roasting temperature is 850℃,roasting time is 3h,leaching temperature is 90℃,leaching agent concentration is 2 mol/L,leaching time is 2h,and leaching L/S is 3.