Codeposition of hydrogen with beryllium, carbon and tungsten
Codeposition of hydrogen with beryllium, carbon and tungsten
复制标题
氢与铍、碳和钨共沉积
DOI:
10.1016/0022-3115(95)00239-1
复制
发表时间:
1996
影响因子:
3.1
通讯作者:
C. M. Frey
中科院分区:
文献类型:
--
作者:
M. Mayer;R. Behrisch;H. Plank;J. Roth;G. Dollinger;C. M. Frey
The trapping of energetic deuterium codeposited with beryllium, carbon and tungsten has been measured on a silicon collector probe at room temperature. The subsequent release of the trapped deuterium at elevated temperatures was determined by thermal desorption spectroscopy. At room temperature, deuterium codeposits both with carbon and BeO with a ration of 0.41 D-atorns/C-atom and 0.38 D-atoms/BeO, respectively. No codeposition of deuterium with tungsten is observed. The thermal release of codeposited hydrogen from BeO begins at 400 K. All hydrogen is released at temperatures above 800 K.